Validation of a Conditioning and Rupture Test Method for Pulmonary Valve Cusps

In surgery, replacement tissues may be used as allografts or autografts. During the Ross procedure, the patient’s own pulmonary valve replaces the diseased aortic valve, and a donor pulmonary valve is placed in the pulmonary position (American Heart Association). The goal of this case study is to develop a reproducible test to characterize the tensile strength of these tissues and examine changes in samples that have undergone a sterilization treatment. The mechanical comparison focuses on whether treated tissue maintains its structural integrity relative to untreated tissue; it does not establish immune compatibility or clinical performance.

The Mach-1 v500c (Biomomentum Inc.) was used to perform puncture testing of porcine pulmonary leaflets using a circular aperture. These tests can be used to analyze the elastic characteristics of the stress-strain curve as well as continue through to failure. A total of 6 porcine hearts were dissected to obtain the leaflets of the pulmonary valves providing 18 samples to be tested. The hearts were frozen on dry ice for transport, placed in a -20°C freezer for storage, and the leaflets were extracted after thawing for 30 minutes in room temperature PBS. This was deemed satisfactory according to O’Leary (2014), as freezing samples was found to not significantly change the mechanical properties of heart tissues. The leaflets were secured in a puncture fixture with a 5mm aperture and punctured with a 4mm spherical ruby indenter (Figure 1). The top of the sample and fixture were used as a basin to hold room temperature PBS to prevent drying. The indenter was lowered and raised through three conditioning cycles for a quasi-static indentation test at a speed of 25 mm/min to reach a tension force of 500 gf. The samples were unloaded and allowed to rest for 5 minutes to return to an unstretched state before the rupture test was performed at the same velocity. The force and displacement data were recorded for further analysis. These methods were adapted from Ragaert (2012), as they were testing leaflets in the aortic position instead of pulmonary. Among the 18 samples tested, 12 specimens (belonging to 4 pulmonary valves of 4 animals, Figure 2) were differentiated by their position within the valve; left (N=4), right (N=4) and anterior (N=4) cusps, to determine if there was any difference between the groups. The other 6 samples were tested, but the position was not identified.
The resultant stress-strain curves show consistency across 17 of the 18 samples, as one was excluded for early rupture. The data was graphed by force versus displacement, and multiple parameters were extracted: stiffness of each conditioning cycle, stiffness of rupture curve, maximum elongation at rupture and maximum load (Figure 3). The data consistently showed repeatable experiments as evidenced by the low standard deviation and coefficient of variance (Table 1).
A one-way ANOVA on the 12 samples with identified positions revealed no significant differences in any studied parameters for the three different positions of the leaflets within the pulmonary valve (Table 2), indicating that it is unnecessary to account for the anatomical position of leaflets within the valve during sample dissection. Future experiments on human pulmonary leaflet samples pre- and post-sterilization can use this finding to help determine the required number of samples for statistical significance. Thus, minimizing the number of animals and cost for a study.
Authors:
Logan Atkinson1, 2, Jasmine Doan3, Nicholas Gilbert3 & Martin Garon3
1. University British Columbia, Cardiac Surgery 2. McGill University, Experimental Surgery 3. Biomomentum Inc.
References:

Figures

Pulmonary valve leaflet mounted over an aperture beneath a spherical indenter.
Figure 1 — Show caption

Pulmonary valve leaflet mounted over an aperture beneath a spherical indenter.

Pulmonary valve leaflet specimens prepared for mechanical testing.
Figure 2 — Show caption

Pulmonary valve leaflet specimens prepared for mechanical testing.

Force-displacement curves for cyclic indentation conditioning and the subsequent rupture test.
Figure 3 — Show caption

Force-displacement curves for cyclic indentation conditioning and the subsequent rupture test.

Top and bottom views of the leaflet puncture fixture during indentation.
Figure 4 — Show caption

Top and bottom views of the leaflet puncture fixture during indentation.

Summary tables of conditioning stiffness and rupture parameters, including comparisons by leaflet position.
Figure 5 — Show caption

Summary tables of conditioning stiffness and rupture parameters, including comparisons by leaflet position.

Find Your Testing Solution

Explore preconfigured testers

Report a problem with this page

Your email is used only to follow up on this report.

Screenshots (optional)

Click this area and paste a screenshot, or drag files here. Up to 3 PNG, JPEG or WebP images; 5 MB per image. Hide confidential information first.

Please do not include passwords or customer information. Reports and screenshots are private.