Skip to content

Indentation Mapping on 36 Pig Skins for a Full Thickness Excision Model

A world-wide renowned Pharma needed to mechanically characterize the healing of skin in a model of full thickness excision. To address their needs, we designed a study to perform the mechanical characterization of the samples the client sent to us. This characterization used two test configurations, namely indentation mapping and tensile testing.

Indentation mapping is a non-destructive technique in which automated indentation is performed throughout the surface of the sample. This technique has several advantages: it is non-destructive and allows the same sample to be used for other tests (e.g. tensile testing in this case) or characterization (e.g. histology). From the recording of each indentation, several mechanical properties can be obtained including the thickness, the structural stiffness and the instantaneous shear modulus. Combined with the positional information of each recording, the topography of the skin can be obtained and distinctive maps for each mechanical properties can be calculated. For this pilot study, maps for the thickness, structural stiffness and the instantaneous shear modulus were generated. From these maps, the area of the “wound” or the “affected skin” were assessed.

Due to the non-invasive nature of the indentation, the second approach used in this study was to perform tensile testing on the same sample to determine the load at rupture.

Following the completion of this pilot study, several other studies were conducted for this client using these characterization techniques.

Figures

Indentation probe contacting a porcine skin specimen.
Figure 1 — Show caption

Indentation probe contacting a porcine skin specimen.

Surface photographs, maximum load maps and thickness maps of two skin scars.
Figure 2 — Show caption

Surface photographs, maximum load maps and thickness maps of two skin scars.

Mach-1 setup for automated indentation mapping of porcine skin.
Figure 3 — Show caption

Mach-1 setup for automated indentation mapping of porcine skin.

Top views of two scars with corresponding cross-sectional surface profiles.
Figure 4 — Show caption

Top views of two scars with corresponding cross-sectional surface profiles.

Skin specimens prepared for tensile testing and the associated gripping fixture.
Figure 5 — Show caption

Skin specimens prepared for tensile testing and the associated gripping fixture.

Find Your Testing Solution

Explore preconfigured testers

Report a problem with this page

Your email is used only to follow up on this report.

Screenshots (optional)

Click this area and paste a screenshot, or drag files here. Up to 3 PNG, JPEG or WebP images; 5 MB per image. Hide confidential information first.

Please do not include passwords or customer information. Reports and screenshots are private.